Rheological properties |
C | Melt volume-flow rate | 260 °C; 5 kg | cm³/(10 min) | ISO 1133-1 | 15 |
C | Molding shrinkage, parallel | 60x60x2; 250 °C / WZ 80° C; 600 bar | % | ISO 294-4 | 0.8 |
C | Molding shrinkage, transverse | 60x60x2; 250 °C / WZ 80° C; 600 bar | % | ISO 294-4 | 0.8 |
| Post- shrinkage, parallel | 60x60x2; 120 °C; 4 h | % | ISO 294-4 | 0.7 |
| Post- shrinkage, transverse | 60x60x2; 120 °C; 4 h | % | ISO 294-4 | 0.7 |
Mechanical properties (23 °C/50 % r. h.) |
C | Tensile modulus | 1 mm/min | MPa | ISO 527-1,-2 | 2400 |
C | Yield stress | 50 mm/min | MPa | ISO 527-1,-2 | 45 |
C | Yield strain | 50 mm/min | % | ISO 527-1,-2 | 2.9 |
C | Nominal strain at break | 50 mm/min | % | ISO 527-1,-2 | >15 |
C | Charpy impact strength | 23 °C | kJ/m² | ISO 179-1eU | N |
C | Charpy impact strength | -30 °C | kJ/m² | ISO 179-1eU | 170 |
C | Charpy notched impact strength | 23 °C | kJ/m² | ISO 179-1eA | 10 |
C | Charpy notched impact strength | -30 °C | kJ/m² | ISO 179-1eA | <10 |
| Izod impact strength | 23 °C | kJ/m² | ISO 180-1U | N |
| Izod impact strength | -30 °C | kJ/m² | ISO 180-1U | 150 |
| Izod notched impact strength | 23 °C | kJ/m² | ISO 180-1A | 10 |
| Izod notched impact strength | 0 °C | kJ/m² | ISO 180-1A | 11 |
| Izod notched impact strength | -30 °C | kJ/m² | ISO 180-1A | <10 |
| Flexural modulus | 2 mm/min | MPa | ISO 178-A | 2500 |
| Flexural strength | 2 mm/min | MPa | ISO 178-A | 75 |
| Flexural strain at flexural strength | 2 mm/min | % | ISO 178-A | 5.0 |
| Flexural stress at 3.5 % strain | 2 mm/min | MPa | ISO 178-A | 70 |
| Ball indentation hardness | | N/mm² | ISO 2039-1 | 104 |
Thermal properties |
C | Melting temperature | 10 °C/min | °C | ISO 11357-1,-3 | 225 |
C | Temperature of deflection under load | 1.80 MPa | °C | ISO 75-1,-2 | 75 |
C | Temperature of deflection under load | 0.45 MPa | °C | ISO 75-1,-2 | 95 |
| Vicat softening temperature | 50 N; 120 °C/h | °C | ISO 306 | 118 |
C | Coefficient of linear thermal expansion, parallel | 23 to 55 °C | 10-4/K | ISO 11359-1,-2 | 0.8 |
C | Coefficient of linear thermal expansion, transverse | 23 to 55 °C | 10-4/K | ISO 11359-1,-2 | 1.0 |
C | Burning behavior UL 94 | 1.5 mm | Class | UL 94 | V-0 |
C | Burning behavior UL 94 | 0.75 mm | Class | UL 94 | V-0 |
C | Burning behavior UL 94-5V | 1.5 mm | Class | UL 94 | 5VA |
| Resistance to heat (ball pressure test) | | °C | IEC 60695-10-2 | 115 |
| Glow wire test (GWFI) | 0.75 mm | °C | IEC 60695-2-12 | 960 |
| Glow wire test (GWFI) | 1.5 mm | °C | IEC 60695-2-12 | 960 |
| Glow wire test (GWFI) | 3.0 mm | °C | IEC 60695-2-12 | 960 |
| Glow wire test (GWIT) | 0.75 mm | °C | IEC 60695-2-13 | 800 |
| Glow wire test (GWIT) | 1.5 mm | °C | IEC 60695-2-13 | 800 |
| Glow wire test (GWIT) | 3.0 mm | °C | IEC 60695-2-13 | 800 |
Electrical properties (23 °C/50 % r. h.) |
C | Relative permittivity | 100 Hz | - | IEC 60250 | 3.3 |
C | Relative permittivity | 1 MHz | - | IEC 60250 | 2.9 |
C | Dissipation factor | 100 Hz | 10-4 | IEC 60250 | 250 |
C | Dissipation factor | 1 MHz | 10-4 | IEC 60250 | 140 |
C | Electric strength | 1 mm | kV/mm | IEC 60243-1 | 30 |
C | Comparative tracking index CTI | Solution A | Rating | IEC 60112 | 300 |
Other properties (23 °C) |
C | Density | | kg/m³ | ISO 1183 | 1310 |
| Bulk density | | kg/m³ | ISO 60 | 800 |
Processing conditions for test specimens |
C | Injection molding-Melt temperature | | °C | ISO 294 | 250 |
C | Injection molding-Mold temperature | | °C | ISO 294 | 60 |
Processing recommendations |
| Drying temperature circulating air dryer | | °C | - | 100 |
| Drying time circulating air dryer | | h | - | 4-8 |
| Residual moisture content | | % | Acc. to Karl Fischer | 0.00-0.02 |
| Melt temperature (Tmin - Tmax) | | °C | - | 240-260 |
| admissible residence time at Tmax | | min | - | <5 |
| Mold temperature | | °C | - | 60-80 |