Rheological properties |
C | Molding shrinkage, parallel | 60x60x2; 280 °C / MT 80 °C; 600 bar | % | ISO 294-4 | 0.32 | |
C | Molding shrinkage, transverse | 60x60x2; 280 °C / MT 80 °C; 600 bar | % | ISO 294-4 | 0.40 | |
| Post- shrinkage, parallel | 60x60x2; 120 °C; 4 h | % | ISO 294-4 | 0.03 | |
| Post- shrinkage, transverse | 60x60x2; 120 °C; 4 h | % | ISO 294-4 | 0.06 | |
Mechanical properties (23 °C/50 % r. h.) |
C | Tensile modulus | 1 mm/min | MPa | ISO 527-1,-2 | 20000 | 12000 |
C | Tensile Stress at break | 5 mm/min | MPa | ISO 527-1,-2 | 225 | 145 |
C | Tensile Strain at break | 5 mm/min | % | ISO 527-1,-2 | 2.4 | 3.5 |
C | Charpy impact strength | 23 °C | kJ/m² | ISO 179-1eU | 90 | 90 |
C | Charpy impact strength | -30 °C | kJ/m² | ISO 179-1eU | 90 | 90 |
C | Charpy notched impact strength | 23 °C | kJ/m² | ISO 179-1eA | 16 | 23 |
C | Charpy notched impact strength | -30 °C | kJ/m² | ISO 179-1eA | 16 | 15 |
| Izod impact strength | 23 °C | kJ/m² | ISO 180-1U | 80 | 80 |
| Izod impact strength | -30 °C | kJ/m² | ISO 180-1U | 80 | 80 |
| Izod notched impact strength | 23 °C | kJ/m² | ISO 180-1A | 16 | 20 |
| Izod notched impact strength | -30 °C | kJ/m² | ISO 180-1A | 16 | 15 |
| Flexural modulus | 2 mm/min | MPa | ISO 178-A | 19300 | 12800 |
| Flexural strength | 2 mm/min | MPa | ISO 178-A | 365 | 235 |
| Flexural strain at flexural strength | 2 mm/min | % | ISO 178-A | 2.8 | 3.6 |
| Flexural stress at 3.5 % strain | 2 mm/min | MPa | ISO 178-A | | 235 |
C | Puncture maximum force | 23 °C | N | ISO 6603-2 | 1250 | 1350 |
C | Puncture maximum force | -30 °C | N | ISO 6603-2 | 1100 | 1150 |
C | Puncture energy | 23 °C | J | ISO 6603-2 | 3.1 | 4.7 |
C | Puncture energy | -30 °C | J | ISO 6603-2 | 2.2 | 2.2 |
| Ball indentation hardness | | N/mm² | ISO 2039-1 | 255 | 155 |
Thermal properties |
C | Melting temperature | 10 °C/min | °C | ISO 11357-1,-3 | 222 | |
C | Temperature of deflection under load | 1.80 MPa | °C | ISO 75-1,-2 | 213 | |
C | Temperature of deflection under load | 0.45 MPa | °C | ISO 75-1,-2 | 220 | |
| Vicat softening temperature | 50 N; 120 °C/h | °C | ISO 306 | 210 | |
C | Coefficient of linear thermal expansion, parallel | 23 to 55 °C | 10-4/K | ISO 11359-1,-2 | 0.12 | |
C | Coefficient of linear thermal expansion, transverse | 23 to 55 °C | 10-4/K | ISO 11359-1,-2 | 0.75 | |
Electrical properties (23 °C/50 % r. h.) |
C | Relative permittivity | 100 Hz | - | IEC 60250 | 5.3 | 11.2 |
C | Relative permittivity | 1 MHz | - | IEC 60250 | 4.7 | 5.1 |
C | Dissipation factor | 100 Hz | 10-4 | IEC 60250 | 164 | 2149 |
C | Dissipation factor | 1 MHz | 10-4 | IEC 60250 | 177 | 651 |
C | Volume resistivity | | Ohm·m | IEC 62631-3 | 5.8E12 | 8E9 |
C | Electric strength | 1 mm | kV/mm | IEC 60243-1 | 33 | 33 |
C | Comparative tracking index CTI | Solution A | Rating | IEC 60112 | 600 | |
Other properties (23 °C) |
C | Water absorption (Saturation value) | Water at 23 °C | % | ISO 62 | 3.6 | |
C | Water absorption (Equilibrium value) | 23 °C; 50 % RH | % | ISO 62 | 1.3 | |
C | Density | | kg/m³ | ISO 1183 | 1700 | |
| Bulk density | | kg/m³ | ISO 60 | 750 | |
Processing conditions for test specimens |
C | Injection molding-Melt temperature | | °C | ISO 294 | 280 | |
C | Injection molding-Mold temperature | | °C | ISO 294 | 80 | |
Processing recommendations |
| Drying temperature dry air dryer | | °C | - | 80 | |
| Drying time dry air dryer | | h | - | 2-6 | |
| Residual moisture content | | % | Acc. to Karl Fischer | 0.05-0.15 | |
| Melt temperature (Tmin - Tmax) | | °C | - | 270-290 | |
| Mold temperature | | °C | - | 80-120 | |